Stainless Steel - Grade 304
CS 304 / 304L Technical Data
Grade 304 stainless steel is the most versatile and the most widely used of all stainless steels. Its chemical composition, mechanical properties, weldability and ncorrosion/oxidation resistance provide the best all-round performance stainless steel at relatively low cost. It also has excellent low temperature properties and responds well to hardening by cold working. If intergranular corrosion in the heat affected zone may occur, it is suggested that CS 304L be used.
Typical Applications
CS 304 is used in all industrial, commercial and domestic fields because of its good corrosion and heat resisting properties. Some applications include:
- Tanks and containers for a large variety of liquids and solids.
- Process equipment in the mining, chemical, cryogenic, food, dairy and pharmaceutical industries.
Chemical Composition (ASTM A240)
- SX
- 304
304L
- °C
- 0.08 max
0.08max
- Mn
- 2.0
max
- P
- 0.045
max
- S
- 0.030
max
- Si
- 1.0
max
- Cr
- 18.0 to
20.0
- Ni
- 8.0 to 10.50
8.0 - 12.0
Typical Properties in
the Annealed Condition
The properties quoted in
this publication are typical of mill production
and unless indicated should not be regarded as guaranteed
minimum values for specification purposes.
1.
Mechanical Properties at Room Temperature
- Tensile Strength, MPa
- Proof Strength, (Offset 0.2%), MPa
- Elongation (Percent in 50mm)
- Hardness (Brinell)
- Endurance (fatigue) limit, MPa
- 304
- TypicalMinimum
- 600515
- 310205
- 6040
- 170-
- 240-
- 304L
- TypicalMinimum
- 590485
- 310170
- 6040
- 170-
- 240-
2. Properties at elevated temperatures
All these values refer to grade 304 only.
Grade 304L values are not given because its strength decreases markedly above 425oC.
Time Elevated Temperature Tensile Strength
- Temperature, °C
- Tensile Strength, MPa
- 600
- 380
- 700
- 270
- 800
- 170
- 900
- 90
- 1000
- 50
Creep data Stress
for a creep rate of 1% in 10 000 h.
- Temperature, °C
- Stress, MPa
- 550
- 120
- 600
- 80
- 650
- 50
- 700
- 30
- 800
- 10
Maximum Recommended Service
Temperature
(Oxidising Conditions)
Continuous
Service
925oC
Intermittent Service
850oC
3.
Properties at Sub-Zero Temperatures
( SX
304 / 304L )
- Temperature
- Tensile Strength
- Proof Stress(Offset 0.2%)
- Impact Strength(Charpy V-Notch)
- °C
- MPa
- MPa
- J
- -78
- 1100/950
- 300/180
- 180/175
- -161
- 1450/1200
- 300/200
- 160/160
- -196
- 1600/1350
- 400/220
- 155/150
4. Corrosion Resistance
Aqueous
As a rough guide the following examples are given for certain pure acid-water mixtures:
- Temperature °C
- Concentration, % by mass
- Sulphuric Acid
- Nitric Acid
- Phosphoric Acid
- Formic Acid
- 20
- 10 20 40 60 80 100
- 2 2 2 2 1 0
- 0 0 0 0 2 0
- 0 0 0 0 0 2
- 0 0 0 0 0 0
- 80
- 10 20 40 60 80 100
- 2 2 2 2 2 2
- 0 0 0 0 1 2
- 0 0 0 0 1 2
- 0 1 2 2 1 0
Key:
0 = resistant - corrosion
rate less than 100 mm/year
1 = partly resistant -
corrosion rate 100m to 1000 mm/year
2
= non resistant - corrosion rate more
than 1000 mm/year
4.2 Atmospheric
The
performance of SX 304 compared with other metals in various
environments is shown in the following table. The corrosion
rates are based on a 10 year exposure.
- Environment
- Rural
- Marine
- Marine Industrial
- Corrosion Rate (mm/year)
- SX 304Aluminium-3S Mild Steel
- 0.00250.025 5.8
- 0.00760.432 34.0
- 0.00760.686 46.2
Thermal Processing
1. Annealing.Heat from 1010oC to 1120oC and cool rapidly in air or water.The best corrosion resistance is obtained when the final annealing is above 1070oC and cooling is rapid.
2. Stress relieving.CS 304L can be stress relieved at 450-600oC for one hour with little danger of sensitisation. A lower stress relieving temperature of 400oC maximum must be used.
3.
Hot working
Initial forging and pressing:
1150to 1260oC
Finishing temperature:
900 to 925oC
All hotworking operations should be followed by annealing.
Note: Soaking times to ensure uniformity of temperature are
longer for stainless steels than for carbon steels - approximately
12times.
Cold Working
CS 304 / 304L being extremely tough and ductile, are readily fabricated by old working.Typical operations include bending, forming, deep drawing and upsetting.
TopQuick Links
- Stainless Grades
- 3CR12 - Corrosion Resisting Steel
- Stainless Steel Grade 430
- Stainless Steel Grade 444
- Stainless Steel Grade 304
- Stainless Steel Grade 321
- Stainless Steel Grade 316
- Stainless Steel Grade 309
- Stainless Steel Grade 310
- Stainless Steel Grade 2001
- Stainless Steel Grade 2304
- Stainless Steel Grade 2205
- Stainless Steel Cromanite
- Material Selection
- Stainless Fabrication
- Stainless Surface Finishes
- Cleaning Stainless Steel